LAY-10 Large pads with a full paste aperture¶
| Severity | Status | Implementation |
|---|---|---|
| suggestion | planned | mid, depends on TOOL-3 |
Looks at. Pad sizes, paste layer apertures and margins per pad.
What it catches. Large pads (exposed pads, screw and shield pads, big SMD tabs) whose solder paste aperture covers the whole pad instead of being split into a window-pane pattern.
Why it matters. A full aperture on a large pad prints far more solder than the joint needs. In reflow the excess floats the part (opens on the small pins around an exposed pad), voids, and squeezes out to bridge neighbours. TI's guidance for QFN exposed pads is 50 to 70 % paste coverage; a 1:1 aperture "results in excessive metal volume that can float the part".
Example. B156A's screw pads printed with full paste wetted up and almost shorted to their neighbours (rev B: less paste). On B135B the big pad of D604 needed its solder amount checked, and B153A's hub wanted a little more paste on its pad: the paste on large pads is a choice to make per part, not a default.
How to check. For pads above an area threshold (a few mm²), read the paste layer: a paste margin of zero with no custom paste shapes means a full aperture. Report them, with the exposed pads of QFN/SON parts first.
Fix. Window-pane apertures for 50 to 70 % coverage on exposed pads (per the part's datasheet when it gives one), reduced and split apertures on screw and shield pads; no paste over thermal vias of 0.3 mm or larger unless the datasheet says so.
References. SLUA271 §4.4 (exposed-pad stencil design); KLC F4.4 (no paste over thermal vias of 0.3 mm or larger); B156 rev B and B135 rev C change lists.